September 10, 2010

Subscribe RSS Share Share

Gear Solutions
Related Articles

 

A Solid State of Affairs - This article explains how a solid–state sensor can be used...

 

Bending Fatigue of Surface Densified Gears - A technical paper discussing the effect of root...

 

Acoustic Properties of Industrial Machinery: Part II - The manufacturing environment can be a fairly noisy place,...

 

A Proven Process for Plastics - When plastic is the material, crowned molding can present a...

 

Tips for Tougher Molded Plastic Gears - Plastics are quickly becoming a contender for some power...

 

Calculating Tooth Form Transmission Error - Modifications to KISSsoft’s gear design software has...

 

Harnessing the Horsepower Thief - To achieve a reduction of parasitic friction in automotive...

 

High Performance Gears for Heavy Duty Transmissons - Surface densification and warm compaction lead to greater...

 

Calculating the Inverse of an Involute - In many variations on a central theme, the involute tooth...

 

Reverse Engineering the Right Way - It's an old machine, but it still works... until that...

 

An Animated Approach to Plotting Profiles - Animated simulations of trochoid spiral and epitrochoidal...

 

Making a Case for PVD Recoating Systems - The following is a case study conducted and prepared by...

 

The Attributes of Loaded Gear Tooth Modeling: Part Two - An in-depth understanding of bevel and hypoid gear tooth...

 

Successful Plastic Gear Conversions - Are you thinking of converting, but still sitting on the...

 

The Attributes of Loaded Gear Tooth Modeling: Part One - An in-depth understanding of bevel and hypoid gear tooth...

 

TWIN Blade--A Cut Above the Rest - In the search for optimizing cutting performance, not only...

 

Grinding Guidelines for Superior Surfaces - Take a quick course on the process and materials used in...

 

Are Energy Answers Blowing in the Wind? - Wind farming--already a viable energy source in Europe and...

 

An Optimized Approach to Straight Bevel Gear Design - Exhaustive research supports new methods for designing and...

 

Superior Grinding: Design by Drake - Looking for an affordable, rapid setup alternative to the...

 

Arrow Offers a Stock Solution - With 53 different combinations of carburized ground tooth...

 

Animated CAD Solutions for Gear Mechanism Design - Embracing new technologies places engineers at the center...

 

Polyglycols for Lubricating Large Gear Drives - Long used for the successful lubrication of worm gears,...

 

Direct Gear Design Drives Performance - On custom jobs, consider Direct Gear Design -- an...

 

The Whirling Process for Improved Worm Gears - Modern design, machining, and heat treating amount to huge...

 

Direct Design for High–Performance Gear Transmissions - For demanding applications where custom gearing is...

 

Microgeometry and Bias in Helical Gear Noise Excitations - While excitation usually originates within the gear mesh,...

 

Reducing Gear Whine in Planetary Gear Transmissions - In an article penned by a technical specialist at the Ford...

 

William Crosher: Tooth Tips - You don’t want to compromise a quality gearbox by scrimping...

 

A Cool Approach to Optimized Bearing Performance - In this article Timken provides you with solid advice on...

 

Relative Curvature of Worm & Wheel with Straight Line Generatrix - You’re sure to benefit from reading this fascinating study...

 

Induction Heating for Low-Cost Quality Gears - Ajax Tocco describes how SPF induction gear hardening can...

 

Low Pressure Carburizing for Transmissions - Low pressure carburizing and high pressure gas quenching...

 

Archives > October 2005 > Allaying Failure with Nitrogen Alloy Bearings

Allaying Failure with Nitrogen Alloy Bearings

Better wear reduction and corrosion resistance are just a few of the benefits of using miniature and small-size ball bearings made of new nitrogen alloy steels.

By: Andreas Kopf, Dipl.-Ing

This study shows that a clear reduction of wear and the probability of bearing failures can be achieved for miniature and small-size bearings by utilizing nitrogen alloy steel for rolling bearings. This is the result of tests that were carried out to study corrosion resistance and wear performance during dry running and working life under mixed friction conditions. It was only proven, however, for a combination of different materials (steel rings, ceramic balls) and excluding absolute dry running.

Introduction
Over the decades, the standard steel 52100 (100Cr6, 1.3505) for rolling bearings proved to be excellent regarding wear resistance in ball bearings. For the application of miniature and small size bearings, however, the need for materials with a higher corrosion resistance soon arose because of the application in diverse areas, e.g. in the medical, dental, saltwater, or aeronautics fields. Materials sensitive to corrosion in high precision instrument ball bearings immediately influence the efficiency of the whole component with regard to friction, accuracy of movement, and vibration/noise.

The material AISI 440C (X102CrMo17 1.3543) initially became the standard material in the area of miniature and small-size ball bearings. This material is a corrosion resistant Martensit chromium alloy steel and, because of this, can be hardened to at least 700 HV2, thus meeting the basic demand for low-noise and load-bearing capacity. The relatively good corrosion resistance of the steel 440C is paid for with more-coarse grain structure and with significantly larger carbides. This influences the noise level significantly in the above mentioned area of miniature and instrument ball bearings. That is why some manufacturers, at the end of the 1980s, changed over to the steel X65Cr13 (1.4037, also called 440D or ACD 34, although no official AISI code exists) which, because of a finer structure, combines the corrosion resistance of the 440C steel and the low-noise level of the 52100 chrome steel.

In addition to the above materials, and the possibility of passivating or surface coating, nitrogen alloy steels such as the SV30 steel X30CrMoN15-1 (similar to 1.4108) are now available for application in corrosive media or environments, which excel in the following properties:

  • The corrosion resistance, especially against chloride ions, at a comparable hardenability is significantly improved by partially substituting carbon, which was necessary for hardening of Martensit steels, by nitrogen.
  • The evenly distributed fine nitrides form a very homogenous structural composition (see figure 1). This gives comparable, if not improved, mechanical properties against conventional materials regarding vibration/noise, mixed friction, and over-rolling behavior.

  • This contribution deals with validating these theoretical facts and connections:

  • Investigation of the (tribo-) chemical resistance by salt spray test and in corrosive applications in practice.
  • Wear dimension measurements regarding wear performance in an unlubricated state (primarily avoidance of adhesion by pairs of different materials: steel-ceramics)
  • Investigation of wear influenced working life under mixed friction in high-speed spindle ball bearings.

  • Corrosion Behavior
    Test Performance
    On the one hand, a salt spray test was carried out to DIN 50021 and ASTM-B-117-73 under laboratory conditions (see figure 2) with parameters defined as follows:

  • Focus on chemical durability only: Outer bearing race at standstill
  • Bearing type: 608 (8 x 22 x 7 mm)
  • Salt concentration: 5 percent aqueous NaCl-solution
  • Temperature: 35ƒC
  • Spray mode: continuously

  • On the other hand the corrosion behavior was tested in cooperation with diverse users, e.g. in medical and flow measurement applications. In this case the data of running tests with "unlubricated" hybrid radial deep groove ball bearings (bearing rings from various steels, balls from Si3N4-ceramics), amongst others of the type 682, were collected in blood and tap water conditions.

    Test Results
    The results of the salt spray tests under laboratory conditions are shown in figure 3 during the test and in
    figure 4 by the resulting corrosion rate.

    Furthermore,
    figure 5 shows a comparison of the working life of ball bearings, which in a medical application ran directly in blood. This medium served, at the same time, as "lubrication."

    Result Discussion
    The nitrogen alloy rolling bearing steel SV30 proved to be more corrosion resistant than the steel X65Cr13 which, so far, has been used for this kind of application under laboratory conditions as well as in practice. Already in previous investigations, during the changing over from the steel 440C to steel X65Cr13, a comparable corrosion resistance had been established.

    Corrosion Behavior in an Unlubricated State
    Test Arrangement
    figure 6 shows the test arrangement for measuring the wear rate in dry, full complement hybrid ball bearings.

    The material pairing of steel rings and ceramic balls avoided adhesion by cold welding in the contact area between the bearing components. Furthermore, a cage was omitted in the test design, as pre-tests showed the working life of various cage designs to be very much below the working life of the bearing rings themselves.

    Test Performance
    The following parameters were defined:

  • Bearing type: 6800/001 VAC1 (10 x 19 x 7 mm); full complement, angular contact on the outer ring; not removable
  • Ring material: 52100, X65Cr13, SV30
  • Ball material: Si3N4
  • Number of balls: Z = 17
  • Bearing arrangement: Preload 10 N by wavy washer; DB-arrangement; Locating-/Floating bearing arrangement (Test bearing = Locating bearing, Floating bearing: grease lubricated standard bearing)
  • Speed: n = 5,000 min-1
  • Load: radially: Fr = 10 N by 1kg weight and return pulley; axially: Fa = 10 N by wavy washer
  • Test duration: 150 hours
  • Temperature: Room temperature

  • Test Results
    figure 7 shows, after an operating time of 150 hours, the wear rate and the deviation in micro-gram of the respective pairs of ball bearing rings in correlation to the used material.

    The balls were not included in the measurement of the wear rate in order for the ring material that might be deposited on the ceramic surface not to be taken into account.

    Result Discussion
    Despite the fine and homogenous structure of the nitrogen alloy steel--to be noted: under absolute dry running conditions--there is no improvement in the wear rate compared with the steel X65Cr13. It shows that the standard rolling bearing steel 52100 still has the highest wear resistance. On the other hand, absolute dry running conditions occur only rarely in practice as, mostly at high speed, at least minimal lubrication remains. In vacuum applications, however, solid lubricants are used, and even in floated bearings the medium itself builds up a thin "lubricating film." Therefore, the behavior in the mixed friction area was investigated in addition by the example of "spindle ball bearings of high speed grinding spindles."

    Wear Influenced Working Life of High Speed Spindle Ball Bearings
    Test Arrangement
    High frequency grinding spindles are used for the production of ball bearing rings. These, again, are excellently suitable to test the wear related working life of spindle ball bearings of GRW's own manufacture. The bearings were, therefore, used under defined conditions of a field test in our own production.

    Test Performance
    Dismountable angular contact bearings of the type 607 (7x19x6 mm), with relieved shoulders of the inner ring and solid phenolic retainers, were installed into the HF-spindles of the manufacturer Gamfior in a field test, so far running for two years, and under the following conditions:

  • Ring material: 52100, SV30
  • Ball material: Si3N4
  • Speed range: 120.000-170.000 min-1
  • Lubrication: Electronic minimum air/oil lubricating device, mineral oil
  • Load: Collective load (Field test), axial preload 100 N
  • Bearing arrangement: Locating/Floating bearing, DF-arrangement

  • The criterion for stopping the individual tests was the running noise of the spindles or the resulting loss in manufacturing quality due to wear of the bearings.

    Test Results
    figure 9 shows the resulting, wear related working life in the previously mentioned field test.

    Result Discussion
    In contrast to pure dry running, an improvement in the wear related working life of approximately 30-35 percent due to the use of nitrogen alloy steel can be detected. In the case of mixed friction or minimum lubrication, the homogeneous structure of the SV30 steel has a positive influence on the mechanical properties and the resulting working life of the bearing.

    Summary
    This study shows that a clear reduction of wear and, due to this, a reduction of the probability of bearing failures can be achieved for miniature and small-size bearings by utilizing nitrogen alloy steel for rolling bearings. This is the result of tests which were carried out to study corrosion resistance and wear performance during the dry running and working life under mixed friction conditions. It was proven, however, only for pairs of different materials (steel rings, ceramic balls) and excluding absolute dry running.


    References:
    1) Bartsch, C.: Der Walzlagerstahl der Zukunft (The rolling bearing steel for the future), "Scope", Issue 7/1999
    2) Bayer, O.: Leistungsgrenzen bei W”lzlagern verschoben (Performance limits of rolling bearings moved), "AGT," Issue 4/1999
    3) Bayer, O., Streit, E., und Trojahn, W.: Leistungssteigerung und Wirtschaftlich-keits--verbesserung bei Hochgenauigkeitslagern durch Cronidur® 30 (Performance and economicalness improvement by CronidurÆ 30), "HTM," Issue 55/2000
    4) Burkard, K.: M–gliche Anwendungsgrenzen f¸r Miniatur- und Instrumentenkugel-lager (Possible application limits for miniature and instruments ball bearings), "Feinwerktechnik," Issue 7/1971
    5) Gamfior S.p.A.: Spindelkatalog (Spindle catalogue), Torino
    6) GRW Gebr. Reinfurt GmbH & Co KG: Miniatur- und Kleinkugellager-Katalog (Miniature and small size ball bearing catalogue), Wurz-burg, 1999
    7) FAG Aircraft/Super Precision Bearings GmbH: Ein neuer stickstofflegierter Stahl f¸r W”lzlager (A new nitrogen alloy steel for rolling bearings), "Der Konstrukteur," 1-2/1992
    8) Menzel, J. und Lueg, J.: Stickstofflegierte St”hle f¸r nichtrostende W”lzlager (Nitrogen alloy steels for stainless steel rolling bearings), "Stahl," 106/1994
    9) Muck, G.: Passivieren von Miniatur- und Instrumentenkugellagern (Passivating of miniature and instument ball bearings), "Maschinen-markt," Issue 58/1969

     

     

    About The Author
    Andreas Kopf, Dipl.-Ing is with Gebr. Reinfurt GmbH & Co KG, W¸rzburg. He can be reached at andreas.koepf@grw.de. Visit online at [www.grw.de].
     

     